冷再生机将再生混合料拌和均匀并由振动压路机稳压一遍后,应立即用平地机初步整形。在直线和不设平曲线段,平地机由路肩向路中间刮平;在设的平曲线段,平地机由内侧向外侧进行刮平。
After the cold regenerator mixes the recycled mixture evenly and stabilizes it once by the vibratory roller, the grader shall be used immediately for preliminary shaping. In straight and non-flat curve sections, the grader shall level from the shoulder to the middle of the road; In the set flat curve section, the grader shall level from the inside to the outside.
必要时再返回刮一遍,对于局部低洼处,应用铁镐将表层5cm以上耙松,并用新拌的混合料进行找平。整形的过程中应及时粗细料离析现象。既由人工配合机械把大块没有破碎掉的旧路料掉。整形时应将高处料直接刮出路外,不应形成薄层贴补现象。
If necessary, go back and scrape again. For local low-lying areas, use an iron pick to loosen the surface layer more than 5cm, and use the freshly mixed mixture for leveling. The segregation of coarse and fine materials shall be eliminated in time during the shaping process. The large pieces of old road materials that have not been broken shall be removed manually and mechanically. During shaping, the high materials should be directly scraped out of the way, and there should be no thin layer of patching.
冷再生机租赁厂家提醒您,在初平完成后,由振动压路机高幅/低频稳压一遍,然后由测量工按照质量控制要求分左、中、右三点放样控制标高和横坡度(直线段20米1点,弯道10米一点),进行细致找平,达到调拱度、调坡度的目的。保证平整度、横坡度符合设计要求。
The cold recycling machine rental manufacturer reminds you that after the initial leveling is completed, the vibratory roller will stabilize the high amplitude/low frequency voltage once, and then the surveyor will set out and control the elevation and cross slope at three points, namely, the left, the middle and the right according to the quality control requirements (20 meters and 1 point for the straight section and 10 meters and 1 point for the curve), and carry out fine leveling to achieve the purpose of camber and slope adjustment. Ensure that the flatness and cross slope meet the design requirements.
冷再生机租赁
冷再生机施工过程中要坚持“宁刮不补”的原则,如果要补料的话,当确定要补5cm以上的混合料,补料的时候,需在新补料中多掺水泥并保证含水量,以确保粘结性,碾压的时候能不松散不起皮。
During the construction of the cold recycling machine, the principle of "scraping rather than patching" should be adhered to. If it is necessary to make up, when it is determined to make up more than 5cm of mixture, it is necessary to add more cement and ensure the water content in the new material to ensure the cohesiveness, and it is not loose and peeling when rolling.
做终平工作时,一定要特别小心,确保整个表面刮平,使其纵向顺适,路拱和符合设计要求。不要在低洼处落下刀片,须将局部高出部分刮除并扫出路外,因为这些料与下层料之间是没有粘结力的,碾压的时候容易造成起皮压不住的现象。终平应仔细进行,对于局部低洼之处,不再进行找补,可留待铺筑沥青面层时处理。
During the final leveling work, special care must be taken to ensure that the entire surface is scraped to make it longitudinal and comfortable, and the road camber meets the design requirements. Do not drop the blade at the low-lying place, but scrape and sweep out the locally higher part, because there is no adhesive force between these materials and the lower layer, which is easy to cause peeling and crushing when rolling. The final leveling shall be carried out carefully. For local low-lying areas, no need to make up, but can be left for treatment when paving the asphalt surface course.
找平完毕后进行1-2遍碾压,碾压前如混合料表面风干,可用洒水车喷洒补水,以防压不住。初压时使用高幅/低频振动模式,以便压实层面的下部,随后使用低幅/高频振动模式压实再生层的上部。碾压时应先轻后重,自路边向路中依次碾压,碾压速度应控制在低速度,注意错轮宽度并且不漏压。
After leveling, carry out 1-2 times of rolling compaction. If the surface of the mixture is dried before rolling compaction, spray water with a watering cart to prevent it from being crushed. The high amplitude/low frequency vibration mode is used for initial compaction to compact the lower part of the layer, and then the low amplitude/high frequency vibration mode is used to compact the upper part of the regeneration layer. The rolling shall be carried out from light to heavy, from the roadside to the middle of the road in turn, and the rolling speed shall be controlled at a low speed. Pay attention to the width of the staggered wheels and do not miss the rolling.
因为水泥的关系,在施工期间,从加水拌合碾压成型洒水养护,不得超过4小时。以上就是为大家介绍的有关冷再生机的详细的介绍,希望对您有所帮助。如果您有什么疑问的话,欢迎联系我们http://www.tclqgc.com
Due to the relationship between cement, during the construction period, from mixing with water to rolling and forming, watering and curing shall not exceed 4 hours. The above is a detailed introduction of the cold regenerator for you, and I hope it will help you. If you have any questions, please contact us http://www.tclqgc.com 。

阅读/ Recommended reading

WR530V路面冷再生机是我公司新推出的路面冷再生机,这款产品不同于450和450机型,是一款完全胜任水稳路基冷再生施工的经济型冷再生机,主要技术参数向600机型看齐,产品综合性...

WR2100L冷再生机转子双转速的应用 2024-04-21
沥青路面养护为什么要使用冷再生机? 2024-04-21
你不知道的压路机选型要点 2024-04-11
旧沥青路面冷再生机械如何进行施工? 2024-04-09

产品/ Recommended products